Corners lifting / warping

The part sticks at first, then corners curl upward off the plate. Bottom is concave when removed.

curlingcorners peeling upbottom not flat

Causes, most likely first

Ordered by how often each is actually responsible, not by how interesting it is. Work down the list.

No enclosure on a material that needs one

ABS, ASA, nylon and PC warp open-frame and no setting fixes it. Enclose the printer or switch material — this is physics, not a profile problem.

Part cooling fan too high

Reduce or disable the fan for ABS/ASA. Cooling is what pulls the corners up.

Bed temperature too low

Raise the bed. A hot plate keeps the lower layers above their transition point so stress cannot pull them free.

Calibration step: Set bed temperature and surface prep →

Sharp corners concentrating stress

Add a brim, or add mouse-ear discs at the corners. A brim is the cheapest fix on this entire list.

Large flat footprint

Shrinkage force scales with area. Split the part, or accept a brim.

Open First Layer →