ASA print settings

ASA prints at about 255 °C with a 100 °C bed and 0% part cooling. Usable range 240–270 °C nozzle, 90–115 °C bed. Needs an enclosure.

Acrylonitrile Styrene Acrylate

Starting settings

Nozzle
240–270 °C (start 255)
Bed
90–115 °C (start 100)
Part fan
0–25% (start 0%)
Wall speed
30–50 mm/s
Max volumetric flow
10 mm³/s
Shrinkage
0.7%
Softens at
100 °C
Enclosure
Required
Nozzle size
0.4 mm or larger — 0.4 mm recommended
Nozzle material
Brass is fine
Drying
70 °C for 4 h

Speed

Same as ABS, 30–50 mm/s. Chamber temperature governs success here, not feed rate.

Bed surface

Smooth PEI at 100 °C inside an enclosure.

What bites people

Safety

Open First Layer →